Low Smoke Zero Halogen bestraalde isolearjende kabelmateriaal (LSZH bestraald isolearjend kabelmateriaal)
PRODUKTEIGENSKIPPEN
GEBRUKSOFTRUIK
Test items en noarmen
Ynspeksje item | Ienheid | Reasken | |||
WDZ-Y-J70 | WDZ-Y-H70 | WDZ-Y-H90 | |||
1 | Treksterkte | MPa | ≥10. 0 | ≥10. 0 | ≥10. 0 |
2 | Ferlinging by brek | % | ≥160 | ≥160 | ≥160 |
3 | Air aging keamer |
|
|
|
|
Aging temperatuer | ℃ | 100±2 | 100±2 | 110±2 | |
Aging tiid | h | 168 | 168 | 240 | |
Maksimum taryf fan feroaring fan tensile sterkte | % | ±25 | ±25 | ±25 | |
Maksimum taryf fan feroaring fan elongation by break | % | ±25 | ±25 | ±25 | |
4 | Termyske deformation |
|
|
|
|
Test temperatuer | ℃ | 90±2 | 90±2 | 90±2 | |
Eksperiminteel resultaat | % | ≤50 | ≤50 | ≤50 | |
5 | 20 ℃ folume wjerstân | Oh · m | ≥1. 0×1012 | ≥1. 0×1010 | ≥1. 0×1010 |
6 | Volumresistiviteit by wurktemperatuer |
|
|
|
|
Test temperatuer | ℃ | 70±1 | - | - | |
Volume resistivity | Oh · m | ≥2. 0×108 | - | - | |
7 | Dielektryske sterkte | MV/m | ≥20 | ≥18 | ≥18 |
8 | Heat shock test |
|
|
|
|
Test temperatuer | ℃ | 130±3 | 130±3 | 130±3 | |
Test tiid | % | 1 | 1 | 1 | |
Eksperiminteel resultaat | - | Gjin kreakjen | Gjin kreakjen | Gjin kreakjen | |
9 | Impact brosheid temperatuer |
|
|
|
|
Test temperatuer | ℃ | -25 | -25 | -25 | |
Eksperiminteel resultaat | Nûmer | ≤15/30 | ≤15/30 | ≤15/30 | |
10 | Ozon ferset test |
|
|
|
|
Test temperatuer | ℃ | - | 25±2 | 25±2 | |
Eksperimint tiid | h | - | fjouwerentweintich | fjouwerentweintich | |
Ozonkonsintraasje | ppm | - | 250~300 | 250~300 | |
Eksperiminteel resultaat | - | - | Gjin kreakjen | Gjin kreakjen | |
11 | Hyt wetter immersion test |
|
|
|
|
Test temperatuer | ℃ | - | 70±2 | 70±2 | |
Eksperimint tiid | h | - | 168 | 168 | |
Maksimum taryf fan feroaring fan tensile sterkte | % | - | ±30 | ±30 | |
Maksimum taryf fan feroaring fan elongation by break | % | - | ±35 | ±35 | |
12 | Oxygen yndeks | % | ≥28 | ≥30 | ≥30 |
13 | Smoke tichtens |
|
|
|
|
flamless | - | ≤350 | ≤350 | ≤350 | |
flaming | - | ≤100 | ≤100 | ≤100 | |
14 | Ferbaarning jout gas acidity |
|
|
|
|
HCI en HBr ynhâld | % | ≤0.5 | ≤0.5 | ≤0.5 | |
HF ynhâld | % | ≤0.1 | ≤0.1 | ≤0.1 | |
pH wearde | - | ≥4.3 | ≥4.3 | ≥4.3 | |
Elektryske conductivity | μS/mm | ≤10 | ≤10 | ≤10 | |
15 | Materiaal reek toxicity gefaren | Neffens de tapassingseasken fan it produkt, ûnderhannele troch de partijen fan oanbod en fraach. |